General
GeneralThe removal of paint and Undercoating by stones chips immediately exposes metal to the atmosphere, causing it to oxidize. The thickness of this oxidation increases if the process continues unchecked. The soft chipping guard primer protects against damage due to the impact of such objects.
Sectional View of Paint Coats:
- The soft chipping guard primer coat is applied over the E.D. (Electrostatically Deposited) primer. It is followed by guide coating and top coating.
- The soft chipping guard primer produces a smooth surface when dry. It should be sprayed so the thickness of the protective film is 20 microns.
Basic Rules for Repairing a Soft Chipping Guard Primer Coat:
- Soft chipping guard primer coat is then applied to the most susceptible area.
- Spray the primer surface (2-part urethane primer surfacer) on the soft chipping guard primer coating areas when you replaced parts using soft chipping guard primer coat." Spray the primer surface (2-part urethane primer surfacer) on the soft chipping guard primer coating areas when you replaced parts using soft chipping guard primer coat.
WARNING:
- Wear goggles or safety glasses to prevent eye injury.
- Ventilate when spraying undercoat.
1. Sanding the replacement part.
NOTE:
- Do not oversand the edges or corners of the part.
- Do not expose base metal.
Use a double action sander and #400 disc sandpaper.
2. Air blowing/degreasing
Use alcohol, and wax and grease remover.
3. Masking
Use masking tape and paper.
4. Spraying primer surfacer
- Spray 4 - 5 coats to get 20 microns of thickness. One coat deposits 5 - 7 microns.
- Do not try to cover the surface with one heavy coat.
Apply several thin coats.
- Use a 2-part urethane primer surfacer and a spray gun.
- Mix the primer surfacer with the additive and solvent, and in the correct ratio.
- Follow the primer surfacer manufacturer's instructions.
5. Drying
After spraying primer surfacer, allow 7 - 10 minutes of drying time, then force dry it with infrared lamps or an industrial dryer.
6. Polishing
Check the primer surfacer has dried thoroughly, then sand the primer surfacer.
Use a double action sander and #400 - #600 disc sandpaper.
7. Intermediate coating and top coating.